| Abstract Scope |
Selective purification of HPAL-derived nickel sulfate solutions requires extensive impurity removal while preserving valuable nickel and cobalt. This study investigates a two-stage CaCO3–MgO neutralization route using oxidized industrial pregnant leach solution. First-stage conditions of 10 wt.% CaCO3, 80°C, 300 rpm, 60 min, and pH 2.90 achieved 93.5% Fe, 51.3% Al, and 58.8% Cr removal, with Ni and Co losses of 5.0% and 0.4%, respectively. The second stage evaluates MgO slurry concentration (2.5–12.5 wt.%), endpoint pH (3.5–4.5), temperature (40–80°C), reaction time (30–150 min), and stirring speed (100–500 rpm). Preliminary results at 5 wt.% MgO showed that lowering pH from 4.50 to 4.00 reduced Ni and Co losses from 31.5% and 21.8% to 12.0% and 10.2%, while maintaining 98.3% Al and 97.6% Cr removal. The study aims to define operating windows for selective impurity control in nickel hydrometallurgical refining. |